Evaluation of fatigue properties of HFIR-irradiated nimonic PE-16 at 4300C

Description

Nimonic PE-16 was irradiated in the HFIR to 6 to 9 dpa and 560 to 1000 at. ppM He at 4300C. Postirradiation fatigue tests revealed a reduction in fatigue life by about a factor of 10 at 4300C. In contrast with AISI type 316 stainless steel, no endurance limit was observed. All irradiated specimens exhibited some intergranular fracture with an increasing tendency toward cleavage like intragranular fracture for low strain ranges

Files

Restricted

The record is publicly accessible, but files are restricted to users with access.

Additional details

Publishing Information

Imprint Title
Alloy development for irradiation performance. Semiannual progress report for period ending September 30, 1983
Journal Page Range
p. 67-71.
Report number
DOE/ER--0045/11