Published 1989 | Version v1
Report Open

Stability of pore size in nuclear track membranes

Description

The stability of pore size in nuclear track membranes from PET was examined by electrical conductance measurements. The membranes were etched and stored under various conditions and the result of the measurements of the pore radius showed that pore size can change after etching when the pores were very small. The decrease of pore size can lead to a complete disappearance when the pore radius after etching was smaller as a critical radius depending on the properties of the initial material, the conditions of the etching process and the storage of the mambranes. 6 refs.; 6 figs

Availability note (English)

MF available from INIS under the Report Number.

Files

22059644.pdf

Files (195.0 kB)

Name Size Download all
md5:a5394102cf189a63979c9cceb8516d33
195.0 kB Preview Download

Additional details

Publishing Information

Imprint Pagination
7 p.
Report number
JINR-E--18-89-794